Stress Relieved Rounds

 

Conforms to:  ASTM A311. 

 

Related Specifications: ASTM A29

 

Chemistry: (Per ASTM A311, Table 1)

Heat Chemical Ranges & Limits, %

UNS Designation

 

Grade

 

Carbon

 

Manganese

 

Phosphorus

 

Sulfur

G11440

1144

0.40-0.48

1.35- 1.65

0.040 max.

0.24 -0.33

 

Mechanical Requirements

 

UNS #

 

Grade Designation

 

Diameter

“s”

 

Tensile Strength

Min, ksi

 

Yield Strength

Min, ksi

 

Elong. in 2 in.

 

Reduction of Area

 

 

 

 

G11440

 

 

 

 

1144

Up to 7/8, incl.

 

105

 

95

 

10

 

30

7/8 to 1-1/4

 

100

 

90

 

10

 

30

1-1/4 to 2

 

95

 

85

 

10

 

25

2 to 3

90

80

10

20

3 to 4-1/2

 

85

 

75

 

10

 

20

Straightness Tolerances(Per ASTM A29, Table A1.14)

Max. of Carbon Range, Under 0.28%

Size, in.

Length, ft.

Rounds

Less than 5/8

Less than 15

3/16

Less than 5/8

15 & over

5/16

5/8 & over

Less than 15

1/8

5/8 & over

15 & over

3/16

 

Size Tolerance * (Per ASTM A29, Table A1.13)

 

 

Size, in.

“s”= diameter

 

1144

Max. of Carbon Range Over 0.28% to 0.55%

To 1-1/2, incl.

0.004

Over 1-1/2 to 2-1/2, incl.

0.005

Over 2-1/2 to 4, incl.

0.006

Over 4 to 6, incl.

0.007

Over 6 to 8, incl.

0.008

Over 8 to 9, incl.

0.009

* Tolerances are minus only, all plus tolerances are 0.

 

 

 

 

 

 

 

 

 

 

                                                                   11

 

 

 

 

 

 

                                                                       

                                                                      

 

 

 